· by Michael Blair, Nashville's Drywall Repair
A bubble in a drywall seam usually turns up at the worst moment, when the second coat goes on or the first coat of paint rolls over it. It looks like a small problem, and it is one, as long as it is fixed under the tape rather than buried under more compound.
What follows is what the gypsum makers list as the causes, how we repair a blister in drywall repair work, and what prevents it on a new seam.
Why is my drywall tape bubbling?
Drywall tape bubbles because it never bonded fully to the compound underneath it. The problems chapter of USG’s CGC Gypsum Construction Handbook lists four causes for blisters in tape: not enough compound under it or compound mixed too thin, tape never pressed into good contact, compound that was too thick and dry, and so much knife pressure that the bed was squeezed out.
National Gypsum describes the same thing from the finisher’s side. Its paper joint tape best practices call the air pockets under paper tape blisters, tell finishers to smooth the tape firmly with the knife while embedding it, and warn that bearing down too hard strips compound from under the tape and leaves a starved joint. Dust on the board is another culprit it names, because it keeps the tape from bonding at all.
Why do bubbles appear after the second coat?
A bubble that shows up under the second coat comes from the first one: every cause USG lists happens when the tape is bedded, so the new coat only reveals a spot that never stuck. USG’s note on joint tapes for paper and mesh says the bedding coat should be thinner than later fill coats and still wet when the tape is pressed in, and that compound which has started to dry leads to blistering under the tape.
Weather is part of it in Middle Tennessee. USG’s handbook ties shrinkage and slow drying to high humidity and to stacking a coat over compound that is not yet dry, and for cold weather it says to hold the room at 55°F or warmer with good ventilation. A room addition or a garage being finished in November without the heat on puts both of those conditions in one room, so we heat the space before taping.
How do you fix bubbling drywall tape?
The fix is to open the blister, put compound back under it and press the tape down again. USG’s remedy is to slit the blistered tape, fill the cut with joint compound, press the tape back in place with the knife blade, and smooth it to a level finish once it has dried.
In practice we cut along the bubble with a sharp utility knife, work compound under both flaps, bed them flat and wipe off the excess without pressing so hard that the bed is gone again. Where the tape has lifted for more than a short run, or has torn, we cut that length out and rebed new tape. Then the seam gets its fill and finish coats as usual and is sanded and primed before paint. A blister under a coat of paint is handled the same way, with a touch-up at the end.
How to keep new tape from blistering
New tape stays down when it is bedded in enough wet, smooth compound, pressed into full contact and given a thin coat over the top. USG’s tape note says to follow the bedding coat with a thin coat over the tape to keep its edges from curling, and warns that piling on too much bedding compound crowns the joint instead. National Gypsum adds clean, dust-free board and fresh compound.
Each coat should dry fully before the next, which USG names as the way to prevent starved joints and delayed shrinkage. The same discipline is behind nail pops and cracked seams that stay fixed. We finish seams on new drywall installation and on repairs in Murfreesboro, Nashville and across Middle Tennessee. To have a bubbling seam looked at, send us a photo and the details.
Sources
- USG (CGC), The Gypsum Construction Handbook, Chapter 12: Problems, Remedies and Preventive Measures — Blisters in tape: causes, the slit-fill-press remedy and prevention; edge cracking and the 55°F cold-weather minimum; shrinkage from slow drying and high humidity; starved joints and drying time between coats.
- USG, Joint Tapes for Industrialized Construction (MH1178) — Bedding coat thinner than fill coats and wet when tape is pressed in; overly dry material leads to blistering; excess bedding compound crowns the joint; thin coat over the tape prevents edge curling.
- National Gypsum, Joint taping tips and techniques for a seamless drywall finish — Air pockets under paper tape called blisters; smooth tape firmly when embedding; excess pressure causes a starved joint; clean, dust-free board and fresh compound.
FAQ
Why Drywall Tape Bubbles, and How to Fix It — questions
Can you put more mud over a drywall tape bubble?
Not if you want it to stay fixed. A blister is tape that is not bonded to the compound under it, so a coat on top only hides it for a while. USG’s remedy is to slit the blister, fill the cut with joint compound, press the tape back down with the knife and smooth it level when dry.
What causes air pockets under drywall tape?
Too little compound under the tape, compound mixed too thin or too stiff, tape not pressed into full contact, or a knife pressed so hard it squeezed the bed out. USG lists those causes for blisters, and National Gypsum adds dust on the board, which stops the tape from bonding.
How wet should joint compound be for bedding tape?
Thinner than the coats that go on later, and still wet when the tape is pressed in. USG’s joint tape note says the bedding coat should have lower viscosity than fill coats and that compound which has started to dry leads to blistering under the tape.
Can you tape drywall in a cold room?
Not well. USG’s Gypsum Construction Handbook says that in cold weather the space should be held at 55°F or warmer with good ventilation while joints are treated, and it links cold, wet conditions to poor bond and cracking along tape edges. Heat the room before taping and keep it heated until the compound dries.